November 16, 2026
What Is Slip Masterbatch, and How Does It Improve the Coefficient of Friction?
The blown film plant won an order from a pet food manufacturer that fills bags on vertical packaging machines and stacks them on pallets with an automatic palletizer. The purchase order said "film with slip", with no further data. To make sure the film would run well, the plant raised the dose of the slip concentrate. On the packaging machine, the film ran flawlessly. On the palletizer, the filled bags slid over one another, the pallet layers shifted and the stretch wrap could no longer hold them. One pallet collapsed inside the truck and dozens of bags arrived torn at the distribution center. The customer's quality department measured the coefficient of friction of the film and found it well below the minimum of its own specification, a range the plant never asked for.
Slip masterbatch is a concentrate that lowers the surface friction of film. Its dose is adjusted so that the coefficient of friction falls within the range your customer requires.
The coefficient of friction, the figure that decides whether the line runs or stops
The coefficient of friction, known as COF, is the ratio between the force needed to slide one surface over another and the force pressing them together. It is a dimensionless number. A low value indicates a surface that runs with little resistance, and a high value indicates a surface that grips.
Static coefficient and kinetic coefficient
The specification distinguishes two values. The static coefficient measures the resistance to start movement, and corresponds to the instant the film starts moving on the machine or a bag begins to slide over another. The kinetic coefficient measures the resistance while the surface is already moving, and corresponds to the continuous travel of the film over guides and formers. The static coefficient is equal to or greater than the kinetic one, and a large difference between them produces jerky travel.
Film to film and film to metal
The same material has different coefficients depending on the surface it rubs against. On the packaging machine, the film runs over the forming collar, the tubes and the steel guides, and there the film-to-metal coefficient is what counts. On the pallet and in the bundle, one bag rests on another, and there the film-to-film coefficient is what counts. In addition, each face of the film can give its own value, because the corona-treated face, the printed face and the sealing face have different surfaces.
What happens when the coefficient of friction falls outside the range
Out-of-specification film fails in either direction, and each direction has its own cost.
High friction: the film drags and the machine loses speed
With a coefficient above the maximum, the film is held back at the forming collar, the pull belts slip and the length of each bag varies. The packaging machine loses speed, wrinkles appear in the seal and the film stretches or tears at the points of greatest tension. That lost production ends in a claim.
Low friction: bags slide and pallets fall apart
With a coefficient below the minimum, the problem appears after the packaging machine. Filled bags slide on inclined conveyors, the pallet layers shift and the stretch wrap loses its grip. Rolls of very slippery film shift sideways as they are wound and form telescoped rolls. This is the case in the opening: a generous dose, applied to secure travel through the machine, left the pallet without stability.
What slip masterbatch is and why it is dosed as a concentrate
Slip masterbatch is a concentrate of slip agent in a carrier resin compatible with your base material. The slip agents most widely used in polyolefins are fatty acid amides. These molecules have low compatibility with the polymer, move to the surface of the film after extrusion and form a very thin lubricating layer that reduces friction.
Oleamide and erucamide, two speeds of effect
Oleamide migrates quickly and lowers friction in the first hours after extrusion, an advantage when the film is converted soon. Erucamide migrates more slowly, reaches a lower final coefficient and better withstands processing temperatures, which is why it is preferred in films that are stored before use or that go through processes involving heat. The choice between them, or their combination, depends on the time between extrusion and use, and on the coefficient that must be reached.
The advantage of dosing slip in masterbatch form
Slip is used in very small amounts relative to the weight of the film, and a minimal variation in dose visibly moves the coefficient. Dosing pure amide at the hopper is impractical and produces areas with excess and areas with no additive. Masterbatch spreads that small amount over a volume of concentrate that is easy to dose accurately, and the film comes out with a uniform coefficient from roll to roll. It also makes it possible to integrate the slip agent and the color in a single concentrate when the film requires it.
The coefficient of friction as a specification figure
An order that says "film with slip" leaves the most important variable open. A useful specification describes the coefficient with five data points, and each one changes the dose of the concentrate.
- 1. The type of coefficient: static, kinetic or both.
- 2. The surfaces in contact: film to film, film to metal, and the face being measured.
- 3. The accepted range, with a minimum value and a maximum value.
- 4. The test method and the conditioning of the sample.
- 5. The age of the film at the time of measurement, counted from extrusion.
A range with a minimum and a maximum
The maximum protects the packaging machine and the minimum protects the pallet. A specification with a single limit invites overdosing, because the plant tries to stay far from the maximum and ends up below a minimum nobody wrote down. The range is defined with the customer, based on their machine, their speed, the product they pack and the way they stack it.
The moment of measurement changes the result
The slip agent keeps migrating for hours and days after extrusion, and the coefficient drops in the meantime. A film measured as it leaves the machine gives a high value that is still going to change. That is why the specification sets the age of the sample and the conditioning, and the plant and the customer measure at the same point in the life of the film. Warehouse temperature also speeds up or slows down migration.
How the coefficient is measured with the sled method
The reference measurement places one film sample on a flat table and another sample around a sled of known weight. An instrument pulls the sled at constant speed and records the force. The initial peak gives the static coefficient and the average force during travel gives the kinetic coefficient. The most frequently cited methods are ASTM D1894, from ASTM International, the U.S. technical standards organization, and ISO 8295, from the International Organization for Standardization.
Variables that move the coefficient even at the same dose
With the dose fixed, the coefficient changes for reasons unrelated to the concentrate. These are the ones we review before adjusting a formula:
- The resin. Migration speed varies among low-density polyethylene, high-density polyethylene and polypropylene, because each resin has a different crystallinity, and many film grades already contain slip from the producer.
- The thickness. A thick film holds a larger reserve of additive and reaches a lower coefficient at the same dose than a thin film.
- The other additives. The silica in the antiblock and high-surface-area pigments adsorb part of the slip agent, and a migratory antistatic competes with it for the surface.
- The film structure. In coextrusion, the slip agent moves from one layer to another, and in laminated film it migrates toward the adhesive, so the coefficient rises after lamination.
- Machine temperature. On hot surfaces, the amide layer softens and friction against metal increases.
How we adjust the dose to the range your customer requires
The adjustment starts from the complete specification and the resin's technical data sheet, to know how much slip the base grade already contains. With that data we choose the amide, or the combination of amides, according to the time between extrusion and use, and we propose a starting dose. The trial film is measured at the age set by the specification, on the surfaces it indicates and with the agreed method. Validation ends on the customer's packaging machine and palletizer, because that is where both limits are confirmed to work.
Slip masterbatch at Delta Pigmentos
At Delta Pigmentos we have been manufacturing masterbatch in our own plant for 24 years. Within our additives line we address slip and blocking requirements, and we formulate the slip concentrate to suit your polymer and your process, in powder or masterbatch form, as a stand-alone additive or integrated into the color of your film. Our Quality Control, Design and Development laboratory reviews with you the resin, the thickness, the additives the formula already contains and the coefficient of friction range your customer requires.
With that information we propose the amide and the dose. You validate the sample in your own production before committing volume. We produce under ISO 9001-2015 certified procedures and ship nationwide from Santa Anita, Jalisco.
Frequently asked questions
What coefficient of friction should you request for your film?
The one your customer's machine and handling require, expressed as a range. The packaging machine sets the maximum and the stacking sets the minimum. That range is agreed with the customer, along with the type of coefficient, the surfaces, the test method and the age of the sample.
Why does the coefficient of friction change days after the film is produced?
Because the slip agent keeps migrating to the surface for hours and days after extrusion. The coefficient drops as the lubricating layer forms, at a rate that depends on the amide, the resin, the thickness and the warehouse temperature.
Can film with friction that is too low be corrected?
In the following lots, yes: the concentrate dose is reduced, the slip already present in the resin is reviewed or the amide is changed, and the film is measured again at the age set by the specification. In a lot that has already been produced, the slip layer remains on the surface, and the solution is agreed with the customer according to its use.
Slip masterbatch turns the coefficient of friction into a controlled figure, within the range that protects your customer's packaging machine and pallet. At Delta Pigmentos we help you define the amide and the dose, with our own laboratory and ISO 9001-2015 certified procedures. Request your quote through WhatsApp or our contact form with your resin, your process, the film thickness and the coefficient of friction range your customer requires; our laboratory will respond with a technical proposal. Every request is reviewed within the following 24 business hours.